文章摘要
肖强伟,张光,鞠忠强,等.石墨铸型材料对钛合金内环铸件冶金质量的影响研究[J].精密成形工程,2018,10(5):143-147.
XIAO Qiang-wei,ZHANG Guang,JU Zhong-qiang,et al.Effect of Graphite Casting Material on Metallurgical Quality of Titanium Alloy Inner Ring Castings[J].Journal of Netshape Forming Engineering,2018,10(5):143-147.
石墨铸型材料对钛合金内环铸件冶金质量的影响研究
Effect of Graphite Casting Material on Metallurgical Quality of Titanium Alloy Inner Ring Castings
投稿时间:2018-06-05  修订日期:2018-09-10
DOI:10.3969/j.issn.1674-6457.2018.05.024
中文关键词: 石墨铸型材料  钛合金铸件  冶金质量
英文关键词: graphite casting materials  titanium alloy castings  metallurgical quality.
基金项目:
作者单位
肖强伟 1. 北京百慕航材高科技股份有限公司北京 1000942. 中国航发北京航空材料研究院北京 1000953. 北京市先进钛合金精密成型工程技术研究中心北京 100094 
张光 1. 北京百慕航材高科技股份有限公司北京 1000942. 中国航发北京航空材料研究院北京 1000953. 北京市先进钛合金精密成型工程技术研究中心北京 100094 
鞠忠强 1. 北京百慕航材高科技股份有限公司北京 1000942. 中国航发北京航空材料研究院北京 1000953. 北京市先进钛合金精密成型工程技术研究中心北京 100094 
赵瑞斌 1. 北京百慕航材高科技股份有限公司北京 1000943. 北京市先进钛合金精密成型工程技术研究中心北京 100094 
王德季 1. 北京百慕航材高科技股份有限公司北京 1000942. 中国航发北京航空材料研究院北京 100095 
摘要点击次数: 3476
全文下载次数: 2628
中文摘要:
      目的 研究不同石墨铸型材料对钛合金内环铸件冶金质量的影响。方法 试验选取颗粒直径分别2, 0.8, 0.04 mm的3种典型石墨材料,制备内环石墨铸型,采用离心浇注,然后对3种不同石墨材质研制的ZTC4钛合金铸件进行表面目视检验、荧光和X光检测。结果 2, 0.8, 0.04 mm这3种颗粒直径的石墨铸型材质研制的铸件表面外观和荧光质量依次提高,其中荧光缺陷平均数量依次为21.4, 13.9, 2.2个/件;铸件内部缺陷数量均小于1.5个/件,夹杂均小于0.7个/件。结论 不同颗粒度直径的石墨铸型对铸件的外观和荧光质量会产生显著的影响,而对铸件内部冶金质量影响较小。
英文摘要:
      The paper aims to study influences of different graphite casting materials on metallurgical quality of titanium alloy inner ring castings. Three typical graphite materials with a particle diameter of 2, 0.8 and 0.04 mm were selected to prepare inner ring graphite casting. Centrifugal casting was used. Then, surface visual inspection, fluorescence and X light detection were carried out on three kinds of ZTC4 titanium alloy castings with different graphite materials. The surface appearance and fluorescence quality of the three kinds of graphite cast moulds with particle diameter of 2, 0.8 and 0.04 mm were improved in turn. The average number of fluorescence defects in the casting was 21.4, 13.9 and 2.2 no./pc in turn; the internal defect of the castings was less than 1.5 no./pc, and the inclusion was smaller than 0.7 no./pc. Graphite mold with different particle diameters has a significant effect on the appearance and fluorescence quality of castings, but has little effect on the inner metallurgical quality of castings.
查看全文   查看/发表评论  下载PDF阅读器
关闭

关于我们 | 联系我们 | 投诉建议 | 隐私保护 | 用户协议

您是第12287105位访问者    渝ICP备15012534号-6

>版权所有:《精密成形工程》编辑部 2014 All Rights Reserved

>邮编:400039 电话:023-68679125传真:02368792396 Email: jmcxgc@163.com

>    

渝公网安备 50010702501719号